MIG welding for beginners comes down to four things: choose the right shielding gas and set enough flow, set a voltage and wire speed pair that suits the plate thickness, hold the gun at the right angle with a short, steady wire stick-out, and listen to the arc to fine-tune. MIG welding (Vietnamese welders often call it "CO2 welding") makes the first bead easier than stick welding because the wire feeds itself, but it also makes it easy to lay a bead that looks good and has not fused. This lesson is written the way a lead welder coaches an apprentice, with a reference settings table and a worked example calculating wire and gas for a box-section steel table frame.
By the end of this lesson, you will be able to:
- Choose CO2 or an Ar/CO2 mix, set the flow rate and check for gas leaks before welding.
- Fit the wire spool, drive roll, contact tip and polarity correctly, and set drive-roll tension so the wire feeds smoothly.
- Set voltage and wire speed for the steel thickness, then fine-tune by the sound of the arc.
- Hold the gun angle, stick-out, push or pull direction and travel speed for an even, fused bead.
- Recognise 6 common MIG faults and calculate wire and gas for a specific job.
Learning to weld properly? MIG/MAG welding for structural steel is step 5 of the roadmap, after arc safety, reading drawings, cutting and fitting, and stick welding. See the 8-step welder roadmap to learn in the right order.
What is MIG welding, and how is it different from stick?
MIG/MAG welding is arc welding with a metal wire fed continuously through a welding gun, while a stream of shielding gas from the nozzle protects the weld pool. The wire is both the electrode and the filler metal. The machine holds the voltage almost constant, and the wire feeder pushes the wire out at the speed you set.
MIG, MAG and "CO2 welding"
- MIG (inert gas): uses argon, mainly for aluminium and some non-ferrous metals.
- MAG (active gas): uses CO2 or an argon + CO2 mix for carbon steel; this is the "CO2 welding" of Vietnamese workshops.
- In this lesson, "MIG welding" follows the everyday workshop meaning: solid wire with gas for structural steel.
Why workshops like MIG
No stopping to change rods, no chipping slag after every bead, and on thin sheet and box section it is many times faster than stick welding. The trade-offs: MIG hates wind (gas blown away means instant porosity), the machine and accessories are more complex, and "cold lap" (filler sitting on the surface without fusing into the base metal) is very hard to spot by eye. If you are already steady with stick welding, as in Stick welding for beginners: set amps, strike the arc, run a bead, you will pick up MIG faster because you already know how to read a weld pool.
Preparing the machine, wire and shielding gas
A MIG set consists of a power source, a wire feeder (built in or separate), a welding gun, a work clamp, and a gas cylinder with a regulator and flow meter (Figure 1). Most beginner problems come from setting up, not from the hand.
Photo: Luke Haggart / Wikimedia Commons, CC BY-SA 4.0
Fitting the wire and setting the drive roll
- Choose a common carbon steel solid wire (AWS type ER70S-6), 0.8 mm diameter for sheet and thin box section, 1.0 mm for 3–6 mm steel.
- The drive roll must match the wire size, with a V groove for steel wire. The contact tip must match the wire too; a worn, oversized tip makes the arc erratic.
- Cut off the bent end of the wire and thread it through the guide into the drive roll and out through the gun. Keep the gun cable straight while threading.
- Set the drive-roll pressure just right: pull the trigger with the wire against a piece of wood; the roll should slip without crushing the wire (Figure 2). Too tight crushes and tangles the wire; too loose makes it feed in jerks.
Photo: dave_7 from Lethbridge, Canada / Wikimedia Commons, CC BY-SA 2.0
Polarity
Solid wire with gas uses reverse polarity: the gun (wire) on the positive terminal, the work clamp on negative. Many machines can swap polarity for gasless flux-cored wire, which is usually connected the other way round. Read the diagram inside the machine cover and the instructions on the spool; wrong polarity gives heavy spatter and poor fusion.
Choosing the shielding gas
| Gas | Advantages | Disadvantages | Use for |
|---|---|---|---|
| 100% CO2 | Cheap, deep penetration, easy to buy | More spatter, rougher bead surface | Structural steel, general fabrication shops |
| 80% Ar + 20% CO2 (or similar) | Smooth arc, little spatter, neat bead | More expensive than CO2 | Thin sheet, work that must look good with little grinding |
| 100% Ar | Inert, does not react | Not suitable for carbon steel | MIG welding aluminium (a later step) |
Gas flow is usually around 12–18 litres per minute indoors out of the wind (Figure 3). More is not better: turbulent gas draws air into the weld pool. CO2 cylinders should have a heated regulator, because expanding CO2 cools and can freeze the regulator during long runs. Brush soapy water on every connection to check for leaks whenever you change a cylinder.
Photo: Mimzy / Wikimedia Commons, CC0
Setting voltage and wire speed
The two most important knobs on a MIG machine are voltage (V) and wire speed (m/min). Understand what each one does and you will set up far faster than by turning knobs at random.
What each knob does
- Wire speed sets the current: faster wire means the machine has to burn more wire, so current rises, penetration deepens and heat increases.
- Voltage sets the arc length: higher voltage gives a longer arc and a wide, flat bead; lower voltage gives a short arc and a narrow, tall bead.
- The two knobs work as a pair: raise the wire speed and you usually need to raise the voltage too. Many newer machines have a synergic (one-knob) mode, but you should still understand the principle so you can fine-tune.
Reference settings for carbon steel, flat position
| Steel thickness | Wire diameter | Voltage | Corresponding current | Notes |
|---|---|---|---|---|
| 1–2 mm | 0.8 mm | 16–18 V | About 60–100 A | Stitch or tack-weld to avoid burning through |
| 3 mm | 0.8–1.0 mm | 18–20 V | About 100–140 A | One pass for fillet welds |
| 5–6 mm | 1.0 mm | 20–23 V | About 150–200 A | Bevel butt joints, possibly two passes |
| 8–10 mm | 1.2 mm | 24–28 V | About 200–280 A | Bevel, multi-pass, machine must have enough capacity |
These are starting points, not answers. The chart inside the machine cover and the wire maker's instructions come first; then run test beads on scrap of the same thickness and fine-tune.
Listen to the arc to fine-tune
- An even crackle like frying bacon: the pair is right; the wire is shorting into the pool steadily.
- Popping, the gun kicking back, wire stubbing into the plate: wire speed too high for the voltage. Lower the wire speed or raise the voltage.
- A long hiss, a big flaring arc, wire burning back to the tip: voltage too high or wire speed too low. Lower the voltage or raise the wire speed.
Gun angle, stick-out and running the bead
With correct settings but a wrong hand, the weld still fails. Three things must stay constant along the bead: gun angle, stick-out and travel speed.
Stick-out
Stick-out is the length of wire from the contact tip to the arc; keep it around 10–15 mm for 0.8–1.0 mm solid wire. Pull the gun back and the wire gets longer, resistance rises, current drops, the arc weakens and gas coverage suffers, so porosity appears. Beginners tend to lift the gun without noticing as their arm tires: rest your wrist or elbow on the bench to hold the distance.
Gun angle and direction
- Work angle: for butt joints hold the gun square to the plate; for fillet (T) joints hold about 45°, splitting the two plates evenly.
- Travel angle: about 10–15°. More than that weakens gas coverage and increases spatter.
- Push or pull: pushing (gun pointed forward) gives a flatter bead and a clear view of the joint edges, good for thin sheet; pulling gives deeper penetration and a taller bead. Slag-producing flux-cored wire is usually pulled.
Travel speed and arc position
Keep the arc on the leading edge of the weld pool; do not let the pool run ahead of the wire. Too fast gives a thin, humped bead with unfused toes; too slow piles up metal, overheats and burns through thin sheet. On 1–2 mm sheet, weld short sections or spaced stitches, let them cool, then join them, to avoid distortion and holes.
Photo: William M. Plate Jr. / Wikimedia Commons, Public domain
Welding positions
Beginners practise in this order: flat (fillet 1F, butt 1G), then horizontal, then vertical, then overhead. Vertical welding on thin sheet is often done downhill for speed and fewer holes; steel 5 mm and thicker is welded uphill for fusion. See Figure 4: the welder wears a helmet and leather gloves and lets the sparks fly away from the body.
Safety when MIG welding
MIG produces a very bright arc with strong ultraviolet light, metal fumes, and adds a high-pressure gas cylinder. General arc safety (helmet, clothing, fire prevention) is covered at the start of the roadmap; below are the points specific to MIG.
Safety warning: Always use a welding helmet with a filter of about shade 10–13 depending on current, safety glasses underneath, leather gloves, long sleeves in cotton or flame-resistant fabric (never synthetic), and safety boots; hang curtains so people nearby are not flashed. Cylinders must stand upright, chained to a wall or cart, with the valve closed during breaks; never weld or strike an arc on a cylinder. CO2 and argon are heavier than air and can cause suffocation in pits, tanks and closed rooms: ventilate and have someone watching. Welding galvanised or painted steel gives off toxic fumes that cause metal fume fever: grind the coating off the joint and use fume extraction or a welding fume respirator. Clear flammable material within about 10 m, keep a fire extinguisher at hand and watch the area for at least 30 minutes after welding. Switch the machine off before changing tips, threading wire or opening the casing.
Checks before every shift
- Gun and earth cables with no cracked insulation, tight connections; work clamp on clean metal close to the weld.
- Nozzle clean of spatter, contact tip not worn, gas flowing when you pull the trigger.
- The work area is dry; never stand on a wet floor while welding.
Common MIG welding faults and how to fix them
Porosity
Sign: tiny holes on or inside the bead. Cause: empty cylinder, gas flow too low or too high, wind, a nozzle full of spatter, a leaking gas hose, oil, rust or paint on the plate. Fix: check gas at the gun tip, screen out wind, clean the nozzle, grind the plate clean.
Cold lap and lack of fusion
Sign: the bead looks round and neat, but its edges sit on top of the plate and may break off under a hard blow. Cause: current too low for the thickness, travelling too fast, letting the pool run ahead of the arc, stick-out too long. Fix: raise wire speed and voltage per the table, keep the arc on the leading edge of the pool, and do bend tests to check.
Heavy spatter
Sign: metal beads stuck all round the weld. Cause: voltage too low for the wire speed, wrong polarity, too much gun angle, dirty plate; pure CO2 naturally spatters more than mixed gas. Fix: reset the pair, check polarity, reduce the travel angle, use mixed gas when appearance matters.
Undercut and burn-through
Sign: a groove along the edge of the bead, or holes in thin sheet. Cause: voltage too high, travel too slow, the gun lingering in one spot. Fix: reduce settings, travel faster, stitch-weld thin sheet.
Bird-nesting at the drive roll and wire fused to the tip
Sign: wire tangles into a ball at the drive roll, or the wire end melts onto the contact tip. Cause: drive roll too tight, dirty or kinked liner, wrong tip size, stick-out too short or voltage too high. Fix: adjust roll pressure, blow out the liner, fit the right tip, keep stick-out at 10–15 mm.
Worked example: welding a 40 × 40 × 2 mm box-section table frame
A workshop is making a workbench frame from 40 × 40 mm square tube, 2 mm wall. The frame has 12 joints, each welded all round the tube. The MIG machine uses 0.8 mm wire and CO2.
Choosing settings
- 2 mm steel, 0.8 mm wire: from the table, about 17–18 V, wire speed about 4.5 m/min (roughly 90 A), gas 15 litres per minute.
- Run test welds on two scrap tube offcuts, listen for an even crackle, and bend-test for root fusion before welding the frame.
- Tack each joint in 4 places, check squareness with a square, then weld side by side, alternating joints diagonally to limit distortion.
Calculating wire and gas
- Weld length: each joint 4 × 40 = 160 mm; 12 joints × 160 mm = 1,920 mm = 1.92 m.
- At a travel speed of about 30 cm/min, arc-on time is 1.92 ÷ 0.30 = 6.4 minutes.
- Wire fed: 4.5 m/min × 6.4 min = 28.8 m. 0.8 mm steel wire weighs about 3.95 g/m, so 28.8 × 3.95 ≈ 114 g. Add 30% for tacks, failed starts and trimmed wire ends: 114 × 1.3 ≈ 148 g, rounded to 0.15 kg.
- Gas: 15 L/min × 6.4 min = 96 litres; add 50% for pre-flow, post-flow and setting up: 96 × 1.5 = 144 litres, roughly 0.29 kg of CO2 (1 kg of CO2 gives about 500 litres of gas).
Welding consumables cost (2026 reference prices, varying by area)
| Item | Quantity × unit price | Amount |
|---|---|---|
| 0.8 mm welding wire | 0.15 kg × 50,000 VND | 7,500 VND |
| CO2 gas | 0.29 kg × 12,000 VND | 3,500 VND (rounded) |
| Contact tips, grinding discs, anti-spatter wear | Estimate | 15,000 VND |
| Electricity | About 0.3 kWh | 1,000 VND (rounded) |
| Total welding consumables | 27,000 VND | |
Check: 7,500 + 3,500 + 15,000 + 1,000 = 27,000 VND (just over 1 US dollar). The lesson in the number: wire and gas for a table frame cost very little; the real cost is the labour of cutting, fitting, welding, grinding and painting. That is why good MIG welders are paid well for working fast without rework, not for saving a few hundred grams of wire. Wire, gas and electricity prices vary by supplier and time.
Frequently asked questions
Is MIG welding harder than stick welding?
Running a first bead is easier, because you do not have to keep feeding a rod down. But setting the machine, managing gas and avoiding cold lap need more understanding. Welders already steady with stick usually reach an acceptable MIG standard after a few dozen hours of practice.
Are CO2 welding and MIG welding the same?
Workshops use the names interchangeably. Strictly, welding steel with CO2 or mixed gas is MAG; MIG uses an inert gas such as argon, mainly for aluminium. Gun technique and machine setup are basically the same.
Can you MIG weld without gas?
Not with solid wire; it will be full of porosity. Self-shielded flux-cored wire welds without gas and suits windy outdoor work, but it is smokier, leaves slag to chip, and is usually connected with the opposite polarity to solid wire.
How much does a small MIG welder for beginners cost?
As a 2026 reference in Vietnam, a home or small-workshop MIG machine of about 200 A taking 1–5 kg spools costs roughly 4–10 million VND depending on brand and features, not including the gas cylinder. Beginners should practise at a vocational school or a workshop with a mentor before buying a machine.
Practice exercises and self-assessment
- Fit a 0.8 mm spool, set the drive-roll pressure, set gas to 15 L/min and check for leaks with soapy water.
- On 3 mm plate, run 3 beads with three different setting pairs, and note the arc sound and bead shape for each.
- Weld 2 T-fillet samples in 5 mm steel, one pushing and one pulling, then cut or bend them to check fusion.
- Calculate wire and gas for 20 joints in 30 × 30 mm box section, using the method in the example above.
Self-assessment criteria
- Pass: the wire feeds smoothly without jerking, gas flow is correct, no leaks at the connections.
- Pass: beads are even in width, with no porosity or undercut; bend tests show metal fused into the root of both plates.
- Pass: your calculation gives 20 × 4 × 30 = 2,400 mm = 2.4 m of weld, and the wire and gas figures add up.
- Not yet: beads that look good but break off at the toe in a bend test (cold lap), or welding without checking gas and wind.
Once your MIG welding on carbon steel is steady, move on to the next step of the roadmap: TIG welding stainless steel and aluminium, and pipe welding in difficult positions, where you learn more precise heat control with a filler rod and TIG torch.
Keep learning to weld: after MIG/MAG come TIG welding of stainless and aluminium, pipe welding in difficult positions, a gate or roof-truss project, and welding certification. See the 8-step welder roadmap.