A weld symbol is an arrow with a horizontal reference line on a drawing that tells you which side to weld, what type of weld it is (fillet or butt), how big and how long it must be, and which process to use. Reading the symbol correctly is only half the job: you also need to know whether the part is carbon steel, stainless steel or aluminium so you can pick the right rod, wire and shielding gas, otherwise a good-looking weld can still crack or rust. This lesson follows the order of work in a real shop and ends with a complete worked example on a steel bracket.
By the end of this lesson, you will be able to:
- Tell carbon steel, stainless steel and aluminium apart in the shop, and explain why each is easier or harder to weld.
- Read the title block and general notes to find the material and welding process on a fabrication drawing.
- Read fillet and butt weld symbols in both the AWS and ISO systems: weld side, leg size z, throat a, length, root gap and bevel angle.
- Choose rods, wire and shielding gas for carbon steel, 304/316 stainless and aluminium.
- Work out the total weld length and the amount of electrode for a part, with figures that add up.
Learning to weld in the right order? Materials, drawings and weld symbols are step 2 of the roadmap, right after arc safety and before cutting, bevelling and tack-up. See the 8-step welder roadmap to see where you are.
Three common material groups and their weldability
"Weldability" means how easy or hard it is to weld a metal into a strong, crack-free joint. In Vietnamese workshops you will mostly meet carbon steel, stainless steel and aluminium.
Carbon steel and carbon equivalent
Steel for frames, gates and brackets is usually low-carbon steel, sold under grades such as SS400 (Japan), Q235 (China), A36 (USA) or the old shop name "CT3 steel". It is easy to weld with stick or MAG. The more carbon and alloying elements, the more the zone next to the weld hardens and the more likely it is to suffer cold cracking; machine shafts, tool steel and leaf springs are hard to weld.
For a quick estimate, engineers use the carbon equivalent from the International Institute of Welding (IIW): CE = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15, where each symbol is the weight percentage on the material certificate. A common rule of thumb: a CE of about 0.40 or lower usually welds well; 0.40–0.60 may need preheating and low-hydrogen rods; above 0.60 needs a dedicated procedure. These are reference thresholds only; the project's approved welding procedure specification (WPS) is the final word.
Stainless steel: poor heat conduction, high expansion, hates iron contamination
In Vietnam you often meet grade 201 (railings, cheap household goods), 304 (water tanks, kitchens, food), 316 (chemicals, coastal sites) and 430 (decorative sheet, magnetic). Grades 304 and 316 weld well; the L versions (304L, 316L) have less carbon to limit corrosion next to the weld. Stainless conducts heat about three times worse than carbon steel and expands about 1.5 times more, so thin sheet distorts fast if you weld in one long run.
The edges of a stainless weld turn yellow, purple and blue (Figure 1); this oxide layer reduces corrosion resistance, so food and chemical work must be cleaned with a stainless brush, pickling paste or electrochemical cleaning. Never use brushes or grinding discs from black steel on stainless: iron dust turns into rust spots.
Photo: Tanel Eensoo / Wikimedia Commons, CC BY-SA 3.0
Aluminium: light, fast heat conduction and a stubborn oxide layer
Aluminium weighs about a third as much as steel, conducts heat about four times faster and melts at about 660°C, while its surface oxide melts at about 2,000°C. If the oxide is not broken up (AC TIG, or thorough cleaning before MIG), the metal underneath melts but the weld does not fuse. Aluminium also does not glow red before it melts, so it is easy to blow holes.
Sheet grades 5052 and 5083 and extrusions in 6061 and 6063 can be welded with the right filler; 6061 welded without filler cracks very easily; 7075 can hardly be arc welded at all, so refer it to the engineer.
| Property | Low-carbon steel | 304/316 stainless | 5xxx, 6xxx aluminium |
|---|---|---|---|
| Magnet | Strongly attracted | Hardly attracted (may be slightly at bends) | Not attracted |
| Weldability | Good (low CE) | Good, but distorts and discolours | Harder: oxide, porosity, burn-through |
| Common processes | Stick, MAG, TIG | TIG, MIG, stainless stick | AC TIG, MIG with argon |
| Post-weld cleaning | Chip slag, anti-rust paint | Remove heat tint, dedicated tools | Dedicated stainless brush |
Identifying material when the paperwork is unclear
Large projects come with a mill certificate showing grade and chemical composition; repair jobs often give you nothing but the piece in front of you.
Read the markings and run quick tests
- Markings: industrial stainless pipe and sheet are usually printed along the length with the grade (304, 316L or UNS code S31603), size and heat number. Take a photo before cutting, because the marked end is often the first offcut.
- Magnet: carbon steel and 430 stainless are strongly attracted; 304 and 316 hardly at all; aluminium not at all. Grade 201 may be slightly magnetic, so a magnet cannot separate 201 from 304.
- Hand weight and grinding sparks: aluminium bar is clearly lighter; low-carbon steel gives long sparks with few branches, high-carbon steel gives bursting, firework-like sparks. Do not test aluminium on a steel grinding wheel.
When to stop and ask
Castings, machine shafts, springs, heat-treated steel, unknown coatings or two different metals: ask before welding. The wrong rod on cast iron or high-carbon steel can leave cracks that only show once the part is under load.
Reading a welding drawing: title block, views, general notes
The fabrication drawing is your work order: read the title block, views, sections and general notes before you look at weld symbols. For general conventions on scale and line types, see how to read architectural drawings.
Title block and bill of materials
The title block gives the part name, drawing number, revision, scale, units (mechanical drawings usually use mm) and material. The bill of materials lists every plate and bar with size, quantity and grade. Always check you have the latest revision: welding to an old revision is the most expensive mistake there is.
Views, sections and general notes
Sections show bevels, gaps and weld shape most clearly. General notes often say things like "All fillet welds 6 mm leg unless noted otherwise", "Weld to WPS no. …" or "Electrode E7016"; these apply to every weld not marked separately. The WPS states the process, filler metal, current, position and preheat temperature; the welder follows it and does not change it.
Anatomy of a weld symbol in AWS and ISO
You will meet two main systems: the American system in AWS A2.4 and the international system in ISO 2553 (European, Japanese and Korean projects often use ISO or a national standard based on it). They differ mainly in how they show the weld side and dimensions.
Arrow, reference line, tail and weld side
The arrow points at the joint; the side it touches is the "arrow side" and the opposite side is the "other side". The reference line carries the symbol and dimensions, and the V-shaped tail holds the process or WPS number. In AWS, a symbol below the reference line means weld on the arrow side, above means the other side, and both means both sides. In ISO 2553 (common drawing style) there is a solid line and a parallel dashed line; a symbol on the solid line means the arrow side, on the dashed line means the other side, and a symmetrical weld on both sides drops the dashed line.
Common supplementary symbols
- A circle at the bend of the arrow: weld all around (around a pipe, a flange).
- A flag at the bend: field weld, made on site.
- Curved or straight line on the symbol: convex, flush or concave weld face.
- Process numbers under ISO 4063: 111 is manual metal arc (stick), 135 is MAG with solid wire, 141 is TIG. AWS drawings usually write SMAW, GMAW, GTAW.
Fillet weld symbols and leg size
Fillet welds are used for T-joints, lap joints and corner joints. The symbol is a right triangle, always drawn with its vertical leg on the left.
Leg size z and throat thickness a
The leg (z) is the side of the weld triangle measured along each plate face. The throat (a) is the distance from the root to the face of the triangle, the part that carries the load. With equal legs, a ≈ 0.7 × z. AWS writes the leg size to the left of the symbol (6 means a 6 mm leg). ISO puts a letter before the number: z6 is a 6 mm leg, a4 is a 4 mm throat, equal to a leg of about 4 ÷ 0.7 ≈ 5.7 mm, rounded up to 6 mm. Read a5 as a 5 mm leg and the weld is about 30% short of load-carrying section.
Figure 2 shows a slip-on flange welded to a pipe with two fillet welds, one ring outside and one inside. On a drawing this is shown with a fillet symbol plus the weld-all-around circle for each side.
Photo: Maggilautaro / Wikimedia Commons, CC BY-SA 4.0
Continuous and intermittent welds
No length means weld the full joint. Intermittent welds add segment length and spacing, but the two systems write them differently. AWS writes "length-pitch", with pitch measured centre to centre: 50-150 means 50 mm segments with centres 150 mm apart. ISO writes "n × l (e)": 3 × 50 (100) means 3 segments of 50 mm with a 100 mm gap between them; total weld length is 3 × 50 = 150 mm and the whole run is 3 × 50 + 2 × 100 = 350 mm long.
Measuring leg size
Use a fillet weld gauge (a set of leaf gauges or a multi-purpose gauge) to measure leg and throat after welding; in Vietnam these cost about 100,000–400,000 VND (~USD 4–16) depending on type (2026 reference). A weld bigger than the drawing is not "stronger": it wastes rod and distorts the part; a smaller one is too weak. Allowed deviations follow the project's acceptance standard.
Butt weld symbols and edge preparation
A butt weld joins two plates or two pipes end to end, common in beam splices, pipework and tanks. Thick plates must be bevelled so the arc can reach the root. Figure 3 shows a pipe butt joint being welded, with the heat-affected zone clearly discoloured on both sides.
Photo: User:Ytrottier , cropped by user:XcepticZP , rotated by user:Michał Sobkowski / Wikimedia Commons, CC BY-SA 3.0
Bevel types and their symbols
| Butt joint type | Symbol shape | Typical use |
|---|---|---|
| Square (I) butt | Two parallel vertical lines | Thin plate, full penetration without bevel |
| Single V | A V | Medium plate, welded from one side |
| Single bevel (half V) | One vertical and one sloping line | One plate bevelled, one square; T-joints needing full penetration |
| Double V (X) | Two Vs point to point across the reference line | Thick plate welded from both sides, less distortion |
| U and J | A U, a J | Very thick plate, less weld metal |
Root gap, root face, bevel angle
Around a butt weld symbol there are three numbers to read: the root gap (distance between the two edges at the bottom), the root face (the square land left at the root so it does not burn through) and the groove angle (the total included angle of the groove). A single-V joint on 8–12 mm plate welded with stick commonly has a groove angle of about 60°, a 1–2 mm root face and a 2–3 mm gap; the correct figures are the ones on the drawing or WPS. In AWS the root gap is written inside the symbol, the groove angle outside it and the bevel depth on the left.
Choosing rods, wire and shielding gas by material
The filler metal must be compatible with the base metal. The table below lists common choices; check current and positions on the label and the WPS. How to read E6013 and E7016 and how to choose MAG gas are covered in stick welding for beginners and MIG welding for beginners.
| Base metal | Stick electrode | MIG/MAG wire | TIG filler rod | Shielding gas |
|---|---|---|---|---|
| Low-carbon steel (SS400, Q235, A36) | E6013 for light work; E7016, E7018 for structural | ER70S-6 | ER70S-6 or ER70S-2 | MAG: 100% CO2 or Ar + CO2; TIG: 100% argon |
| 304, 304L stainless | E308L-16 | ER308LSi | ER308L | TIG: 100% argon; MIG: argon with about 2% CO2 or 1–2% O2 |
| 316, 316L stainless | E316L-16 | ER316LSi | ER316L | Same as 304 |
| Stainless to carbon steel | E309L-16 | ER309LSi | ER309L | Same as 304 |
| 5xxx aluminium (5052, 5083) | Rarely used | ER5356 | ER5356 | 100% argon |
| 6xxx aluminium (6061, 6063) | Rarely used | ER4043 or ER5356 | ER4043 or ER5356 | 100% argon |
Carbon steel: reading the ER70S-6 wire code
Carbon steel electrodes follow AWS A5.1 (such as E7016), and MAG wire follows AWS A5.18. In ER70S-6, ER means it can be used as an electrode or a filler rod, 70 is a minimum tensile strength of about 70,000 psi, S means solid wire and 6 is the group with more deoxidisers, more tolerant of slightly dirty plate. Low-hydrogen rods (E7016, E7018) must be kept dry and baked as the label says before structural welding (Figure 4).
Photo: Không rõ tác giả / Wikimedia Commons, Public domain
Stainless: the L, grade 309, and no pure CO2
Stainless electrodes follow AWS A5.4 and stainless wire AWS A5.9, and the code starts with the alloy number: 308 for 304, 316 for 316. L means low carbon, and Si helps the weld wet out nicely in MIG. To join stainless to black steel (a stainless railing post onto a steel base plate), use 309L. Do not weld stainless with pure CO2, because the weld picks up carbon and loses corrosion resistance; full-penetration stainless pipe needs an argon back purge so the root does not burn black.
Aluminium: 4043 or 5356
Aluminium wire follows AWS A5.10. ER4043 (aluminium-silicon) flows easily, cracks less and is easier for beginners; ER5356 (aluminium-magnesium) is stronger and matches colour better if the part is anodised later. For 5083 and other high-magnesium grades use 5356, not 4043. Use 100% argon, remove oil with solvent, brush the oxide with a stainless brush kept only for aluminium, and weld within a few hours of brushing.
Safety warning: Stainless welding fume contains chromium and nickel; aluminium welding gives off strong ultraviolet light and ozone; galvanised steel fume causes metal fume fever: always use local fume extraction and wear a suitable respirator for long work in enclosed shops. Stainless pickling paste contains strong acids (often hydrofluoric acid): wear chemical-resistant gloves and eye protection, follow the safety data sheet, and if it touches skin, rinse with water at once and seek medical care. Solvents for cleaning aluminium (acetone, alcohol) are flammable; keep them away from the welding area. Review the full basics in welding safety.
Worked example: reading a steel bracket drawing and listing consumables
Loc, a second-month apprentice at a structural shop in Binh Duong, is asked to weld 1 pipe-support bracket: a 300 × 200 × 10 mm base plate, a 200 × 150 × 8 mm upright plate and 2 triangular gussets 8 mm thick. The title block says SS400; the general notes say "Stick welding (111), E7016 ø3.2, fillet welds with natural convex face, no grinding".
Step 1: read the symbols
- Weld A (upright to base plate): ISO symbol z6 with triangles on both sides, length 200: a 6 mm leg fillet weld, both sides, along the full 200 mm; a ≈ 0.7 × 6 = 4.2 mm.
- Weld B (each gusset to the base plate and to the upright): z5 on both sides. Each gusset edge is 100 mm, but the gusset corner has a 10 mm snipe so weld A can run past, leaving 90 mm of weld; a ≈ 0.7 × 5 = 3.5 mm.
- No flag, no circle: shop weld, not welded all around.
Step 2: check the material with the carbon equivalent
The plate certificate shows C 0.16%, Mn 0.90%, Cr 0.02%, Mo 0.01%, V 0%, Ni 0.02%, Cu 0.03%. CE = 0.16 + 0.90/6 + (0.02 + 0.01 + 0)/5 + (0.02 + 0.03)/15 = 0.16 + 0.15 + 0.006 + 0.003 = 0.319, rounded to 0.32. That is below the 0.40 reference threshold for 10 mm plate, so the shop does not require preheat; Loc only needs to bake the rods as labelled and clean rust and oil from the weld area.
Step 3: work out weld length and electrode quantity
| Weld | Length calculation | Length (mm) | Cross-section (mm²) | Volume (cm³) |
|---|---|---|---|---|
| A: z6, both sides | 2 sides × 200 | 400 | 20 | 8.0 |
| B: z5, both sides | 2 gussets × 2 edges × 2 sides × 90 | 720 | 14 | 10.1 |
| Total | 1,120 | 18.1 |
The cross-section of a fillet weld is estimated as z²/2 plus about 10% for convexity: z6 gives 36/2 = 18, times 1.1 is about 20 mm²; z5 gives 25/2 = 12.5, times 1.1 is about 14 mm². Volume: 20 × 400 = 8,000 mm³ = 8.0 cm³ and 14 × 720 = 10,080 mm³ ≈ 10.1 cm³, a total of 18.1 cm³. Multiplied by the density of steel, 7.85 g/cm³, that is about 142 g of weld metal. Stubs, slag and spatter mean a real deposition efficiency of about 60%, so you need about 142 ÷ 0.6 ≈ 237 g of electrodes. Loc takes 0.5 kg of baked rods to cover tack welds and test strikes.
Common mistakes when reading drawings and choosing consumables
- Welding the wrong side: the weld ends up on a face where another plate must fit, while the side that needed it is bare. The cause is mixing up AWS above/below with ISO solid/dashed lines. Fix: confirm the symbol system before tack-up and mark the weld side on the part with chalk.
- Confusing a with z: the measured weld is smaller than required even though the welder "followed the number". When you see a, multiply by about 1.4 to get the leg (a5 needs a leg of about 7 mm) and write the converted figure on the part.
- Using black-steel rod on stainless: the weld shows brown rust after a few weeks. The causes are the wrong rod, shared brushes or discs with black steel, or heat tint left on. Use 308L, 316L or 309L rod and wire as in the table, and dedicated stainless tools.
Frequently asked questions
How do you read a fillet weld symbol?
Find the triangle on the reference line and see which side it is on to know whether to weld the arrow side or the other side. The number on the left is the size (leg z or throat a); the numbers on the right are length and spacing for intermittent welds; no length means weld the whole joint.
What is the difference between leg size and throat thickness?
Leg z is measured along the plate face; throat a is measured from the root to the weld face; with equal legs, a ≈ 0.7z. ISO drawings state a or z explicitly; AWS drawings treat the number on the left as the leg size by default.
Which rod do I use for stainless steel?
Use E308L-16 for 304, E316L-16 for 316 and E309L-16 for stainless to black steel. Thin parts and food-grade work are usually TIG welded.
Practice and self-assessment
- Take 3 offcuts in the shop (steel, stainless and aluminium if available), use a magnet, hand weight and markings to name each one, and write down how you decided.
- Ask for an old fabrication drawing, copy every weld symbol onto paper and note next to each: weld type, weld side, size, length and process.
- Convert a3, a4 and a5 to approximate leg sizes, then measure an existing weld with a fillet gauge.
Self-assessment criteria
- Pass: 3 out of 3 materials named correctly; weld side, size and length correct for every symbol (your supervisor finds no errors when checking); a-to-z conversions within 0.5 mm.
- Not yet: any weld side wrong, a confused with z, or a rod or wire from the wrong material group. Reread the relevant section and repeat with a different drawing.
Once you can read symbols fluently and choose consumables, the next step on the roadmap is Cutting, bevelling & tack-up: turning the root gaps, groove angles and root faces you just read on the drawing into real parts, and tacking them so the weld does not pull the part out of shape.
Keep learning to weld: after materials and weld symbols come cutting, bevelling and tack-up, stick welding, MIG/MAG, TIG on stainless and aluminium, out-of-position welding and weld inspection. See the 8-step welder roadmap.